      Production Process of Carbonized wood outdoor chairs

      "Carbonized wood" gluing properties and surface finishing, good performance, and pine in the heat treatment process, turpentine basically volatile resin has cured, therefore, the resin ducts and Setsuko surface, do not do special sealing process can be directly do finishes. Carbonized wood outdoor chairs in use, it will not happen hot weather resin overflow, destroying the paint surface problems.

      Kiln and tank "carbonized wood" outdoor chair production process are divided into primary drying and secondary drying, charring rapid heating, cooling and conditioning treatment, and then cooling the kiln (tank) 5 phase.

      1 Primary Drying

      From birth (wet) wood dried to approximately 12% (or 10%) moisture phase is called once dry. This stage can be in the kiln carbonization (tank) carried, also accomplished by conventional kiln. Given carbonization kiln (tank) of the cost is higher, and the high cost of equipment operation, so using conventional drying kiln for a more economical, and the drying quality is also easier to control, but the drying time.

      (2) second drying

      From 12% dried to a wood moisture content of 3% (or 4%) of the second drying phase is called. This phase carbonization furnace (tank) to complete. Moisture content of about 12% of the timber into the carbonization kiln, the first transition can be conventional drying. Dry bulb temperature from about 65-75 ℃ Start, and then heated in stages to about 125 ℃, wet bulb temperature gradually expanded to 25 ℃. Subject wood moisture content to about 3%, the secondary drying stage ends. This phase of the length of time, depending on the wood species and thickness, 22mm thick timber normally takes more than 10 hours.

      3 rapid heating carbonization

      Wood moisture content of 3% after, they spent the dry dangerous period. Can quickly heat up, in a relatively short period of time, rising carbonization temperature (usually 180 ~ 212 ℃). Carbonization temperature then held constant for about 3 hours, high temperature heat treatment of wood, the wood of the hemicellulose and amorphous cellulose degradation, wood moisture greatly reduce the number of hydroxyl groups. Meanwhile in wood extractives such as resin, terpenoids, tannins, acids, a large number of objects containing volatile. Thus greatly reduced hygroscopicity of wood, dimensional stability and significantly improved corrosion resistance. This stage, the kiln (tank) to be filled within a protective gas (usually water vapor), oxygen gas must be less than 2%, a simple measure of the kiln to maintain the wet-bulb temperature of 99.5 ~ 100 ℃.Otherwise, there will be very dry wood fire hazard, and the wood under high temperature oxidation, its strength is also unfavorable.

      4 cooling humidity

      Wood carbonization treatment, not only the water content is very low (0.5%), and the wood itself, the temperature is high, close to 180 ~ 212 ℃. Then the humidity can not be directly processed must first timber to cool. Note do not use air cooling, if the kiln outside in the fresh air flow into the kiln, it is easy to make wood fire. The correct way is to stop the radiator heating while spraying atomized water to the kiln, not only play a role in cooling, but also make almost all dry timber proper humidification.Subject to the kiln medium temperature dropped about 116 ℃, humidity conditioning treatment can be carried out. Then the kiln while the saturated water vapor injection, and then atomized water spray in order to enhance the relative humidity of the kiln medium moisture content of wood, and to eliminate the residual stress. Wood moisture content generally be increased from 4 to 5%, to end the humidity treatment.


      CONTACT US

      Contact: Mr Chen

      Phone: 13521257486

      Tel: 010-82921102

      Email: zhitong_chenfei@163.com

      Add: Northwest of Beijing haidian district

      主站蜘蛛池模板: 五月天激情电影| 制服丝袜在线一区| 亚洲国产长腿丝袜av天堂| 18禁无码永久免费无限制网站 | 午夜少妇性开放影院| 久久影库| 少妇人妻真实偷人精品视频| 国产精品久久久久久nⅴ下载编辑| 91高跟黑色丝袜呻吟在线观看| 亚洲欧美综合中文| 成年美女黄的视频网站| 婷婷综合激情| 久久久久久av无码免费看大片| 欧美 日韩 人妻 高清 中文| 色屁屁影院www国产高清麻豆| 97一区二区国产好的精华液| 8x8ⅹ成人永久免费视频| 亚洲一区二区自拍| 放荡的少妇2欧美版| 蜜臀av99无码精品国产专区| www.久草.com| 在线播放免费人成毛片| 亚洲最新中文字幕成人| youjizz国产| 国产系列在线| aⅴ在线视频男人的天堂| 无码草草草在线观看| av福利院| 91精品国产闺蜜国产在线闺蜜| 影音先锋男人av鲁色资源网 | 午夜时刻免费入口| 亚洲日本乱码在线观看| 国产一区二区三区 韩国女主播| 自拍三级| 欧美性日韩| 亚洲日韩在线观看免费视频| 亚洲妇女行蜜桃av网网站| 亚洲不卡在线视频| 免费a级黄毛片| 国产精品爽爽久久久久久无码| 欧美片网站免费|